淡江大學機構典藏:Item 987654321/36020
English  |  正體中文  |  简体中文  |  全文笔数/总笔数 : 64178/96951 (66%)
造访人次 : 10036859      在线人数 : 19704
RC Version 7.0 © Powered By DSPACE, MIT. Enhanced by NTU Library & TKU Library IR team.
搜寻范围 查询小技巧:
  • 您可在西文检索词汇前后加上"双引号",以获取较精准的检索结果
  • 若欲以作者姓名搜寻,建议至进阶搜寻限定作者字段,可获得较完整数据
  • 进阶搜寻


    jsp.display-item.identifier=請使用永久網址來引用或連結此文件: https://tkuir.lib.tku.edu.tw/dspace/handle/987654321/36020


    题名: 都市垃圾焚化反應灰穩定燒結再利用技術之研發
    其它题名: MSWI reaction ash regeneration by stabilization accompany with sintering process
    作者: 劉瓊玲;Liou, Chiung-ling
    贡献者: 淡江大學水資源及環境工程學系碩士班
    高思懷;Gau, Sue-huai
    关键词: 焚化飛灰;水萃;磷酸;穩定;燒結;抗壓強度;回收再利用;Fly ash;washing;Phosphoric acid;stabilization;sintering and regeneration
    日期: 2005
    上传时间: 2010-01-11 07:28:58 (UTC+8)
    摘要: 垃圾焚化後產生大量焚化灰渣,其中飛灰因重金屬溶出量未能符合毒性溶出標準,被歸類為有害廢棄物,需經適當的處理。而飛灰之處理著重在固化與穩定化,但若能再資源化,更可創造新資材。
    本研究先以水洗方式去除飛灰中可溶性物質,增加飛灰後續處理之穩定性,再以磷酸穩定重金屬,以減少重金屬溶出之潛勢,另一方面磷酸亦有助於提升後續燒結資源化之效果,穩定後之水洗灰以燒結熱處理技術將燒製成營建用骨材,以達資源化之目的。
    由實驗結果得知,飛灰經過兩次水萃後,可有效的將易溶出的鹽類先萃出,氯鹽萃出率可達90%,水洗後之飛灰以適量之磷酸溶液做飛灰重金屬穩定處理,可有效降低Pb的再溶出, 使水洗灰符合TCLP標準。水洗灰經磷酸穩定後,添加適量黏土與淨水污泥,以1000與11000C燒結,成品已達營建骨材之條件,具回收再利用之可行性。
    Municipal solid waste treatment method was treading toward incineration in Taiwan. A large amount of fly ash could be produced. The heavy metals concentration of fly ash failed to meet the EPA’s regulation of TCLP test thresholds. The de-toxicfication and stabilization for fly ash were necessary and the final aim is regeneration.
    This study was to develop a new process that could cheaply and stably treat the fly ash and regenerate the products. The process includes water-washing, phosphoric acid stabilization, and sintering. Washing could remove the soluble salts in the fly ash, which is harmful to the sintering process; the phosphoric acid could stabilize the heavy metals. The pretreated fly ash could be safely materialized by sintering technology.
    The study was found that fly ash after water washed twice, the soluble salt could remove 90%. After stabilized with proper dosage of phosphoric acid solution, the concentration of Pb were significantly reduced in the TCLP extract of the washed fly ash samples. Then the stabilized samples were mixed with designed percentage of water purification sludge and clay, and sintering at 1000 and 1100 0C. The sintered products could achieve the criteria for aggregate of construction that is possible to be regenerated.